Properties

F  NAM 39

F NAM 37

F  NAM 30

F  NAM 32

F  NAM 33

 

Specified values

Tested values

Specified values

Tested values

Specified values

Tested values

Specified values

Tested values

Specified values

Tested values

Density (gm/cm³)

1.50 – 1.90

1.76

1.70-2.00

1.79

1.70 – 2.00

1.80

1.70 – 2.00

1.82

1.70 – 2.00

1.85

Tensile Strength (N/mm²)

≥ 6.0

10.83

≥ 7.0

12.50

≥ 10.0

14.35

≥ 14.0

16.35

≥ 12.0

12.70

Compressibility (%)

7 – 15

9.85

7 – 15

9.05

7 – 15

8.36

6 – 12

9.86

6 – 12

10.20

Recovery (%)

≥ 40

63.75

≥ 50

65.30

≥ 50

59.00

≥ 50

64.00

≥ 50

59.86

IN ASTM Oil No. 3

a)      Increase in Mass (%)

b)      Increase in thick. (%)

 

≤ 15.0

≤ 10.0

 

8.15

6.20

 

≤ 15.0

≤ 10.0

 

7.03

5.20

 

≤ 10.0

≤ 10.0

 

6.38

3.27

 

≤ 10.0

  8.0

 

6.88

5.27

 

10 – 30

10 – 30

 

17.32

22.51

IN Fuel ‘B’

a)      Increase in Mass (%)

b)      Increase in thick. (%)

 

≤ 10.0

≤ 10.0

 

6.10

6.48

 

≤ 10.0

≤ 10.0

 

 

5.70

5.20

 

≤ 10.0

≤ 10.0

 

6.67

3.68

 

≤ 10.0

  7.0

 

6.67

4.68

 

10 – 30

10 – 30

 

11.58

15.56

 

IN Water/Antifreeze 50:50

a)      Increase in Mass (%)

b)      Increase in thick. (%)

 

≤ 15.0

  5.0

 

7.83

4.65

 

≤ 15.0

≤ 5.0

 

6.17

4.08

 

≤ 10.0

≤ 5.0

 

7.18

4.22

 

≤ 15.0

  5.0

 

6.18

4.22

 

≤ 15.0

  5.0

 

10.47

4.98

Loss on Ignition %

≤ 40.0

29.65

≤ 28.0

27.92

≤ 36.0

25.50

≤ 30.0

26.50

≤ 35.0

26.43

Tensile Strength decrease

 

36.91

(2.0m)

 

14.28

(2.0m)

 

37.97

(2.0m)

 

21.93

(1.5m)

 

67.29

(1.5m)